English

Burner Liner Assembly Fit: Stock, Datums, Holes

Table of Contents
What part and route were used?
Why did the blank arrive without a usable datum?
How were the datum holes opened first?
How much stock was left on faces and holes?
How were the M4 threads and Ø12 holes proved?
What does this record prove and not prove?
FAQs

The failed casting was recovered by running a printed liner in parallel, not by fixing the casting. This liner was printed with 2.0 mm face stock and 1.0 mm hole stock, datumed on two Ø8H7 holes, then machined to 0.05 mm flatness and ±0.05 mm hole position. The record covers one part and one route; it does not prove a batch, a customer acceptance or a service life.

Printed burner liner blank with datum holes and stock on the assembly faces, before machining

Machined liner with three window frames and the base flange, seen from the open side

What part and route were used?

The part is a burner liner in GH3536, a 1.8 mm wall shell with three window frames, a base flange and 12 M4 holes. The route was laser powder bed fusion, solution treatment, hot isostatic pressing, then five-axis machining from two datum holes.

The blank measured 2.0 mm over the assembly faces and 1.0 mm in the holes. The print was oriented on its base plate so the flange face carried the stock and the window faces stayed vertical. That orientation kept the long open wall out of the recoater shadow and left the flange flat enough to cut a datum.

The heat treatment and the HIP ran before any cut. Solution treatment at 1,180 °C for 1 h released the printing stress, and HIP at 1,180 °C and 100 MPa for 3 h closed the porosity. The blank was scanned after each step, so the cutter received a measured blank rather than a nominal one.

Why did the blank arrive without a usable datum?

The blank arrived without a usable datum because the printed skin is not a datum: it moves with the heat cycles. The as-printed flange face was 0.4 mm out of flat across the 96 mm width, and the two printed datum holes were 0.3 mm off position (case file CL-04).

Using the skin as a datum would have carried that 0.4 mm into every face. The first operation therefore cut the base plate flat to 0.03 mm before opening the datum holes, and the printed skin never touched the fixture.

The stock map from the post-HIP scan showed 2.2 mm at one corner of the flange and 1.7 mm at the opposite corner. That 0.5 mm difference is the thermal movement the scan was there to catch, and it set the depth of the first facing pass. The datum cut was planned before the print was released, so the blank was never routed on the skin.

  1. Print: GH3536 blank with 2.0 mm face stock and 1.0 mm hole stock, built on the base plate.

  2. Heat: solution treatment at 1,180 °C for 1 h, then HIP at 1,180 °C and 100 MPa for 3 h, with a scan after each step.

  3. Measure: post-HIP scan shows 2.2 mm at one flange corner and 1.7 mm at the opposite corner.

  4. Decide: datum cut on the base plate first, then every face and hole from that chain.

How were the datum holes opened first?

The datum holes were opened in the first operation on the flat plate: two Ø8H7 holes at 0.02 mm true position, reamed and checked on a CMM before the second operation started. The plate was clamped on aluminium soft jaws at 0.5 MPa.

The first operation also marked the reference edge and the window side. The second operation bolted the part on the two holes and cut every other feature from that chain: the assembly faces, the three window frames, the Ø12 holes and the M4 threads.

Datum transfer was checked at the end. The hole position held at ±0.05 mm, and the flatness after unclamping read 0.03–0.05 mm. The difference between the in-fixture reading and the released reading was 0.02 mm, which matched the clamp-load prediction for a 1.8 mm wall at 0.5 MPa. The same pair of readings was taken on the third part and repeated inside 0.01 mm.

How much stock was left on faces and holes?

Faces carried 2.0 mm and holes 1.0 mm, read from the post-HIP scan rather than from CAD. The facing pass removed 1.7 mm at the thin corner and 2.2 mm at the thick corner, which brought both faces to the same plane in one setup.

The holes were drilled after the faces, so their position came from the datum and not from the printed skin. The Ø12 holes were drilled and bored to size, and the four M4 holes per window frame were drilled, tapped and gauged in the same setup.

No second roughing setup was needed. The 2.0 mm allowance covered the datum cut, the 0.05 mm flatness and the local warp, and the part came out of the first setup with enough stock for a 0.1 mm finishing pass.

How were the M4 threads and Ø12 holes proved?

Every M4 thread was cut to 1.5×D engagement and checked with go/no-go gauges; every Ø12 hole was checked with a plug gauge and its position on the CMM. The thread inspection was the gate that held the part, not the last operation before shipping.

The M4 holes were tapped at 250 r/min in the same setup as the faces, so a thread that failed could be re-cut before the part left the machine. One hole was re-tapped after the go gauge entered too far; the no-go gauge then held, and the part stayed in the record.

The Ø12 holes were probed after boring. Position held at ±0.05 mm, and the bore diameter held inside the drawing band. The proof was recorded per hole, not per part, because the assembly fit depends on the worst hole rather than the average. The record sheet carried the gauge number and the operator for each row.

Check

Callout

Reading

Datum hole position

0.02 mm

0.01 mm

Face flatness after release

0.05 mm

0.03–0.05 mm

Hole position

±0.05 mm

±0.04 mm

M4 engagement

≥1.5×D

1.5×D, go/no-go pass

Assembly fit band

±0.9 mm

inside band

What does this record prove and not prove?

The record proves that one liner can be cut to 0.05 mm flatness and ±0.05 mm hole position from two datum holes, with 2.0 mm face stock and 1.0 mm hole stock. It does not prove a 20-part batch, a customer acceptance or a service life; those need their own trials and records.

The final acceptance band for the assembly was ±0.9 mm on the fit features, and the part met it with margin. That band is wider than the flatness callout because it describes the assembly, not the machined face.

What the record also shows is where the next part could fail: the thread gate, the clamp load or the datum transfer. Each of those has a number and an inspection, so the next run can be checked against this one rather than against a memory of it.

Send the failed part, the drawing and the assembly fit band. Neway reviews the datum chain against the assembly, returns the stock map and quotes the superalloy 3D printing and CNC machining steps with the inspection gate named. The heat treatment, the hot isostatic pressing and the powder bed fusion build are quoted on the same chain, and the route comparison sits on the Neway blogs page.


FAQs

  1. How tight must burner liner flange flatness be?

  2. Thin wall clamping: what pressure holds the part?

  3. M4 thread in a thin wall: how do you tap it?

  4. Machining stock allowance: how much should stay?

  5. First-article trial cut: how do you prove stability?