Thin wall clamping for a printed liner is set at 0.5 MPa or less on aluminium soft jaws, with the cavity filled in gypsum. The 1.8 mm wall is too flexible for a three-jaw chuck, and the fixture, not the cutter, decides whether the released part still meets 0.05 mm flatness. A clamped part can measure flat and still spring back when the jaws open.
A thin wall moves because the clamp stores elastic energy in the part, and that energy releases when the jaws open. A 1.8 mm GH3536 wall at 0.5 MPa deflects within its elastic range, and the machined face follows that deflection. The face is cut in the clamped shape, so it springs back to the free shape.
The movement is measurable. On this liner the face moves 0.02 mm to 0.05 mm after release, depending on where the jaws sit and how much stock is left. That is the same order as the 0.05 mm flatness callout, which is why the clamp design cannot be separated from the tolerance.
Thin wall clamping also depends on where the part is supported. A jaw that lands on a window frame pinches a stiff rib; a jaw on the open wall bends it. The contact pattern matters more than the tonnage, and a pressure gauge alone does not prove a good setup. A dial indicator on the free face after each pass shows the trend before the finish cut.
0.5 MPa on aluminium soft jaws holds this liner still for roughing, and 0.4 MPa is used for semi-finish and finish passes. The jaws are machined to the part contour so the load spreads over an area rather than a point. Below that pressure the part can chatter; above it the wall deforms and the cut follows the deformation.
The cavity is filled with gypsum before the first cut. Gypsum supports the inside of the 1.8 mm shell, damps vibration and spreads the clamping load, then is broken out and washed after machining. It also gives the part a temporary floor, which helps when the base flange is machined first.
Thin wall clamping pressure is checked on the machine gauge and recorded per part, together with jaw position and contact pattern. A setup that needs 0.8 MPa to stop chatter is already bending the wall, so the answer is a better support, not more force. The superalloy printing route sets the wall, and the fixture has to follow it. Solution treatment runs before machining and fixes the free shape the fixture must hold.
Soft-jaw clamping stops working below 0.8 mm wall thickness, where the jaw pressure needed to hold the part already exceeds what the wall can take. It also fails when the part has no flat land for the jaw, or when the windows leave an unsupported span longer than about 80 mm.
A three-jaw chuck is the wrong tool for this geometry even at 1.8 mm. Point contact on a curved wall makes a local dent, and the dent becomes a flatness error after release. Dedicated soft jaws or a gypsum-filled fixture are the alternatives.
When the wall cannot be supported, the process changes rather than the force. Options include machining in two setups with an intermediate release and re-check, leaving more stock for a final light pass, or moving the datum to a thicker feature. None of them is free, and all of them are cheaper than scrapping a finished liner. A stress-relief pass between roughing and finishing is one of those changes, and it is recorded on the route card.
Send the wall thickness, the window layout and the faces to be machined. We will propose a jaw and support plan, name the clamping pressure, and quote the five-axis machining step against the released flatness. One review covers fixture, stock and inspection; include the flatness callout and the release condition in the request.