Boss position tolerance on a printed transition duct holds ⌀0.10 mm to the machined duct axis. Every part is read on a coordinate measuring machine (CMM) after the two spigots and the eight boss faces are cut, and the callout comes from the spigot diameters rather than from the printed shell. The eight G1/8 bosses sit on a 2.5 mm wall in Hastelloy X (UNS N06002), so the machined axis is the only reference both ends share.
Both ends of the duct are turned in one setup, and that gives the axis a physical definition. The two spigot diameters, ⌀79.7 mm and ⌀100.85 mm, are cut first, the CMM fits an axis to them, and the eight boss positions are reported against it. A boss located from the printed outline inherits the 0.5 mm of ovality that solution treatment leaves in the shell. General tolerances on the unmachined shell stay at ISO 2768-1.
Position and roundness fail for different reasons. A duct that is 0.10 mm oval can still pass a ⌀0.10 mm boss position tolerance once the axis is fitted to the spigots, while a round duct fails position when the fixture springs the wall during the cut. Both numbers come off the same setup, so neither one can hide the other.
The thread carries a second control. Coaxiality of the thread bore to its boss stays inside ⌀0.20 mm, because a G1/8 port loaded off-center preloads one side of a 6 mm boss and starts a crack at the root. Boss faces are cut to 6.0 mm above the axis, so the axial and radial references are set in one clamping.
Every duct is measured, not sampled. The report carries the fitted axis, the eight boss positions and the roundness of both spigots on one page, and the release decision reads that page rather than a single line on it.
Pilot holes finish at ⌀8.8 × 26.4 mm through, bored from the spigot datum in the same setup as the boss faces. The printed hole arrives at ⌀8.4 mm, which leaves 0.2 mm of radial stock for the boring bar.
Boring replaces drilling here because a drilled hole follows the printed wall. The CNC post-machining step starts from that blank, so a printed pilot that sits 0.15 mm off its nominal position is taken out in one pass instead of chased with a second setup.
Bore and thread are cut without re-clamping. Opening the fixture between bore and tap adds close to 0.2 mm of spread on a 2.5 mm wall, twice the position callout, and the tap then drags the hole with it. Thread depth stays at 21.12 mm against a ⌀8.8 mm pilot.
The eight holes are gauged with go/no-go plugs to that 21.12 mm depth. A plug that stops short sends the boss back to the tap, not to the CMM, because the position was already accepted at the bore stage.
A boss goes to review when boss position tolerance passes ⌀0.20 mm, or when the thread bore has broken into the boss wall. Both are checked on the part with the fixture opened, because a clamped measurement hides the movement that produced the error.
Between the callout and the review limit, a boss is re-cut rather than scrapped. Boring and tapping again from the corrected datum recovers the feature while the boss face still holds its 6.0 mm height above the axis and both spigots still clean up to ⌀79.7 mm and ⌀100.85 mm. Each pass takes 0.3 mm, and the fixture holds 0.4 MPa on the spigot land rather than on the 2.5 mm shell.
Two cases sit outside this answer. A boss already welded to close a cleaning hole cannot be re-positioned by machining. A duct whose spigot diameters no longer clean up cannot be corrected by moving the bosses, because the axis itself has moved with them.
A boss measured out of position before solution treatment is not a review case either. The 1180 °C cycle moves the wall again, so position is re-read within 24 h of the furnace run and before any re-cut decision.
Send the duct sketch, the boss pattern and the spigot limits to Neway, and we will set the datum sequence and name the stock left in each pilot hole. The same review covers the datum chain from the spigots to the eight bosses, and prices the superalloy 3D printing blank with the CNC machining step.